ASTM A193 covers several bolting grades that look alike on a drawing but behave very differently in service. B7 is high-strength alloy steel, B8 Class 1 is standard 304 stainless, and B8 Class 2 is 304 stainless that has been strain hardened for strength close to B7 at smaller diameters. B8M is the 316 version. This guide compares strength, corrosion resistance, cost and availability so you can specify – or substitute – the right grade.
| B7 | B8 Class 1 | B8 Class 2 | B8M Class 2 | |
|---|---|---|---|---|
| Material | Alloy steel (4140 / 4142), quenched and tempered | 304 stainless, solution treated | 304 stainless, solution treated and strain hardened | 316 stainless, solution treated and strain hardened |
| Min. tensile | 125 ksi (to 2-1/2″) | 75 ksi | 125 ksi up to 3/4″, falling to 100 ksi at 1-1/2″ | 110 ksi up to 3/4″, falling to 90 ksi at 1-1/2″ |
| Min. yield | 105 ksi (to 2-1/2″) | 30 ksi | 100 ksi up to 3/4″, falling to 50 ksi at 1-1/2″ | 95 ksi up to 3/4″, falling to 50 ksi at 1-1/2″ |
| Corrosion resistance | Low – needs a coating (zinc, galvanizing or similar) | Good | Good | Better in chlorides, salt and de-icing exposure |
| Magnetic | Yes | Essentially no | Slightly, from the cold work | Slightly, from the cold work |
| Matching nut | A194 2H | A194 8 | A194 8 (S1 strain hardened if specified) | A194 8M |
| Relative cost | Lowest | Low | Higher | Highest |
| Availability | Widely stocked | Widely stocked | Limited – often 6–8 weeks elsewhere; Benchmark 14–21 days | Limited – Benchmark 14–21 days |
Strength values are ASTM A193 minimums. Always confirm requirements with the engineer of record.
B8 Class 1 and Class 2 are the same 304 stainless, but Class 2 is cold worked after solution treatment. That strain hardening more than triples the yield strength at small diameters (100 ksi vs 30 ksi up to 3/4″). Swapping in Class 1 to beat a long lead time leaves the connection with a fraction of its design strength – so a substitution always needs the engineer of record’s written approval.
The benefit of strain hardening falls as diameter grows: at 1-3/8″ to 1-1/2″ Class 2 yield is 50 ksi. Check the strength table for your exact diameter, or use the B8 Class 2 torque calculator, which applies the correct strength for each size.
Class 2 bolts are identified by the grade marking with an underline (B8SH underlined) and are supplied with mill test reports confirming the Class 2 properties.
Up to 3/4″, B8 Class 2 matches B7’s 125 ksi minimum tensile with 100 ksi yield (B7: 105 ksi). Above 3/4″ Class 2 strength drops with diameter, down to 100 ksi tensile and 50 ksi yield at 1-1/2″, while B7 stays at 125/105 ksi up to 2-1/2″.
Only if the engineer approves and corrosion is handled another way. B7 is alloy steel and rusts without a coating, so it is not a direct replacement in exposed or wet locations.
B8 is Type 304 stainless; B8M is Type 316, which contains molybdenum for better resistance to chlorides. Strength is slightly lower for B8M Class 2 at small diameters (110 ksi vs 125 ksi tensile up to 3/4″).
ASTM A194 Grade 8 heavy hex nuts, or Grade 8M for B8M. Some specifications call for strain-hardened nuts (Supplement S1). Benchmark supplies all nut types.
Benchmark’s typical lead time is 14–21 days, compared with the 6–8 weeks many suppliers quote, with mill test reports and grade stamping on every order.
Benchmark supplies B8 and B8M Class 2 bolting for bridge bearings and anchor rods, structural steel, pressure piping and valves, water and wastewater treatment, and industrial maintenance. Send your bolt list or call 800-580-4195.